AW1050
Features
Low mechanical strength. High resistance to corrosion. High electrical and thermal conductivity. Easy creation, good weldability.
Routine Use
Chemical, pharmaceutical and food, utensils and appliances, containers, electrical, signs, graduated scales, packaging (tubes, boxes, caps), thin foils, ceilings.
Possibilities of application and use
CRITERIA | ||
CORROSION | Resistance to normal atmosphere | Excellent |
Resistance industrial atmosphere | Excellent | |
ELECTRICAL COND. | Electrical conductivity | Excellent |
SUP. TREATMENT | Polishing | Excellent |
Industrial anodizing | Excellent | |
Decorative anodizing | Excellent | |
CONFORMED | Hot folded | Excellent |
Cold folded | Good | |
Inlaid/repulsed | Good | |
Forged | – | |
Machining | Medium-Bad | |
ASSEMBLY | Welding under protective atmosphere | Excellent |
Resistance welding | Good |
Chemical composition
ELEMENTS | Si | Fe | Cu | Mn | Mg | Cr | Ni | Zn | Ti | Bi | Pb | Al | OTHER |
MINIMUM | – | – | – | – | – | – | – | – | – | – | – | – | – |
MAXIMUM | 0.25 | 0.4 | 0.05 | 0.05 | 0.05 | 0.05 | 0.05 | 0.07 | 0.05 | – | – | REST | – |
% weight
Mechanical features
METALLURGICAL STATUS | Rp 0.2 (MPa) | Rm (MPa) | A50 (%) | Hardness HB |
O/H-111 | 20 | 64-95 | 28 | 20 |
H18 | 120 | 140 | 5 | 44 |
H-24 | 105 | 105-145 | 10 | 36 |
Bending radius
THICKNESS | |||||||
ALLOY/STATUS | 0.4>e<0.8 | 0.8>e<1.6 | 1.6>e<3.2 | 3.2>e<4.8 | 4.8>e<6.0 | 6.0>e<10 | 10>e<12 |
COEFFICIENTS FOLDING | |||||||
0/H111 1050 | 0 | 0 | 0 | 0.5 | 1 | 1 | 1.5 |
H24 1050 | 0 | 0.5 | 1 | 1 | 2 | 2 | 2.5 |
* MULTIPLY BY THE RATIO THICK PLATE AND OBTAIN THE RADIO FOLDING